A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Etching SiO2 without affecting Aluminum
Etching SiO2 without affecting Aluminum
2003-05-15
bobo
2003-05-15
Tobias Kramer
2003-05-15
beaton@npphotonics (Bill Eaton)
2003-05-15
Kirt & Erika Zipf-Williams
2003-05-15
Mark McNie
2003-05-16
Neal Ricks
2003-05-15
Pavel Neuzil
2003-05-15
Dave Kharas
2003-05-16
[email protected]
2003-05-16
David Springer
Etching SiO2 without affecting Aluminum
Pavel Neuzil
2003-05-15
Dear Bobo,
you do not have that many options, oversaturated HF
(between 70 and 80% !!!) can do the job. YOu can
purchase 73% from Fluka but it takes time as it is
classified as weapon (it is used to enrich Uranium),
the other option is Pelchem (www.pelchem.com) from
South Africa. I would go for the later one without any
hesitation. The delivery will be much cheaper and
faster.
Do not forget that the liquid is very dangerous,
really good fllow box is essnetial and you HAVE to use
isopropanol before dipping it into a DI water after
the etching. The whole trick is that the Al must not
get into a contact with diluted HF.
Pavel




________________________________________________
Dear all,
does anyone knows what wet etchant can etching silicon
dioxide without
etching aluminum at the same time?   Thanks.


__________________________________
Do you Yahoo!?
The New Yahoo! Search - Faster. Easier. Bingo.
http://search.yahoo.com

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Nano-Master, Inc.
MEMS Technology Review
Addison Engineering