PECVD Si3N4 recipe
Roger Shile
2003-06-23
A recipe I've used for PECVD SiN on a Pacific Western Systems Coyote is:
330 sccm SiH4 (100%)
2000 sccm NH3
300 watts RF Power
pressure = 2 torr

Roger Shile

----- Original Message -----
From: "Dlee Li" 
To: 
Sent: Friday, June 20, 2003 2:17 PM
Subject: [mems-talk] PECVD Si3N4 recipe


> Hi,
> anyone can give me his workable PECVD Si3N4 recipe? we need to add PECVD
> Si3N4 to our system.
>
> thanks
> Dlee
>
> _________________________________________________________________
> MSN 8 helps eliminate e-mail viruses. Get 2 months FREE*.
> http://join.msn.com/?page=features/virus
>
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Harrick Plasma, Inc.
The Branford Group
Process Variations in Microsystems Manufacturing