Hi Sriram,

You must make sure that the Tri Chloro Ethylene is completely gone from the
surface, other wise you may get a reaction with the HCL that will attack the
interface between the Pt and SiO2. How come you are using boiling TCE (TCE
is a very dangerous solvent pretty much banned here in the USA), there are
better alternatives such as 5:1:1  H2O:H2O2:NH4OH (let the solution cool off
after mixing), the Pt will act as a catalyst and start a very vigorous
reaction, stay in for 5 mins, rinse in DI and N2 dry.

Another caution 3000A Pt maybe under high stress and want to peel off on its
own.

Rick


-----Original Message-----
From: [email protected]
[mailto:[email protected]]On Behalf Of sriramb
Sent: Saturday, July 26, 2003 5:43 AM
To: [email protected]
Subject: [mems-talk] Gold plating


Dear All,

I tried to plate Gold over a Platinum thin film (3000 Angstrom) on SiO2.
Before the plating, we go through a degreasing step, wherein we boil the
Silicon wafers in Tri Chloro Ethylene, followed by a dilute HCl dip.
The Pt film is deposited by DC sputtering.

The trouble is that the Pt film peels off when the HCl dip is done.

What should I do to overcome this problem?

Thanks in advance.

Thanking You,
With Best Regards,
Sriram
Senior Process Engineer,
BEL Bangalore
INDIA



_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Addison Engineering
The Branford Group
MEMStaff Inc.