Al etch
2003-09-09
Sagi Daren
2003-09-09
Kirt & Erika Zipf-Williams
2003-09-10
transene
Al etch
Kirt & Erika Zipf-Williams
2003-09-09
Aluminum Etchant Type A from Transene at 50 C might be selective enough:
Measured etch rates:
Al:     530 nm/min
Al/2%Si: 660 nm/min
Ti:    0 nm/min
Ni:    29 hm/min
TiNi not measured

    --Kirt Williams, Ph.D.    consultant

----- Original Message -----
From: Sagi Daren 
To: 
Sent: Tuesday, September 09, 2003 12:30 AM
Subject: [mems-talk] Al etch


> Hi All
> I am looking for an Aluminum etchant which is highly selective for
> Nickel/Titanium films which lay beneath.
> Have tried some NaOH solutions but they didn't do the work.
> Thank you all for your help
>   S. Daren
>
>       Sagi Daren
> Senior R&D Engineer
>  El-Mul Technologies
> Tel.:972-8-9434184 #43
> [email protected]
>
>
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
Process Variations in Microsystems Manufacturing
The Branford Group
Nano-Master, Inc.