MEMSnet Home: MEMS-Talk: SF6 Glas etching
SF6 Glas etching
2003-09-15
Jim Beall
2003-09-15
Xu Zhu
2003-09-16
Blunier, Stefan
2003-09-16
R. Brent Garber (2 parts)
2003-09-16
Blunier, Stefan
SF6 Glas etching
R. Brent Garber
2003-09-16
Hey folks,

Just to add the little I know into this question.  SF6 tends to leave a film
on the inside of your chamber.  I use it to etch Tungsten.  I also use the
system (Trion minilock RIE) to etch III-V material.  We have found that
doing a high power, high flow O2 run for 5 to 10 minutes after every SF6 run
helped keep our chamber nice and clean between runs.

Brent

"Blunier, Stefan" wrote:

> Hi Jim
> It seems that everybody having a Si etching systems is very anxious to
> try. I haven't got any reply on my question.
> Greetings
> Stefan
>
> -----Original Message-----
> From: Jim Beall [mailto:[email protected]]
> Sent: Montag, 15. September 2003 16:23
> To: General MEMS discussion
> Subject: Re: [mems-talk] SF6 Glas etching
>
> Stefan -
>
> I wonder if you ever received any useful information in response to
> this inquiry?
>
> We also have an STS ASE system and were told to never do anything
> else so as to not disturb the chamber chemistry, but I wonder how
> critical this really is.
>
> Thanks,
>
> Jim
>
> >Dear colleagues
> >>From the publication of Ichiki et al. Thin Solid Films 435 (2003)
> >>62-68
> >I learned that glas
> >etching with SF6 and Ar works quiet well. When we bought 4 years ago a
> >ICP system (STS) for Si deep etching and a RIE system for glas (resp
> >SiO2, Si3N4) etching we were told from STS not to do
> >both processes in the same chamber because of reproducibility.
> >Does anyone has experience in running glas etch (SF6/Ar) and silicon
> >deep etching
> >on the same ICP system. Do I contaminate the si deep etching chamber by
> >glass etching
> >or is it possible to clean up the system without open it (no mechanical
> >clean)?
> >
> >Thanks for response.
> >Greetings
> >Stefan
>
> --
>
>   - Jim Beall 303-497-5989
>     [email protected]
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
garber.vcf (text/x-vcard, 361 bytes)
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
MEMS Technology Review
Tanner EDA by Mentor Graphics
The Branford Group