A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Q: Ti wet etching
Q: Ti wet etching
2003-10-17
t. hamano
2003-10-17
Kirt & Erika Zipf-Williams
2003-10-21
M. Mubeen Almoustafa
2003-10-18
Linda LW Chow
2003-10-18
kris
2003-10-20
Devarajan Balaraman
Q: Ti wet etching
M. Mubeen Almoustafa
2003-10-21
If you are interested in dry etch, then using SF6 at low pressure and
moderate power is the way to go.

Mubeen Almoustafa
Process Engineer
Trion Technology

-----Original Message-----
From: [email protected]
[mailto:[email protected]]On Behalf Of Kirt
& Erika Zipf-Williams
Sent: Friday, October 17, 2003 11:07 AM
To: General MEMS discussion
Subject: Re: [mems-talk] Q: Ti wet etching

> I would like to ask you about the recipe of Ti etchant.  We are going to
> etch a <50 nm thick Ti layer on epitaxial barium titanate.  Since this
> material must be unfamiliar with you, you don't forget about it.  I just
> want to know what kinds of etchant you usually fix for Ti etching.
> Thanks a lot in advance.
> T. Sophie Hamano

You can use 10 H2O : 1 H2O2 (30%) : 1 HF (49%).
My measured etch rate for sputtered titanium is 1.1 um/min = 1100 nm/min.

    --Kirt Williams, Ph.D.    consultant


_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Mentor Graphics Corporation
MEMS Technology Review
Harrick Plasma, Inc.