A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: SU-8 50 wrinkling issue
SU-8 50 wrinkling issue
2003-12-12
[email protected]
2003-12-15
Michael L
2003-12-15
Brubaker Chad
2003-12-15
[email protected]
2003-12-23
[email protected]
2003-12-23
Mighty Platypus
Re: SU-8 50 wrinkling issue
2003-12-25
[email protected]
SU-8 50 wrinkling issue
Brubaker Chad
2003-12-15
First off, I'd like to ask whether you are using a hotplate or an oven to
perform the pre-bake?  The paametes laid down in the data sheets from MicroChem
are for hotplate baking. If you are using an oven, especially for films that
this, you will have a solvent removal issue; the top layer of resist will dry
first, creating a "crust" of densified, low solvent content material.  This will
act as a diffusion barrier to any solvent attempting to escape from the lower
layers.

Even if you are using a hotplate, I think I may see an issue with the prebake
parameters. Your message implies that you are using the original formulation of
SU-8 50, rather than the faster drying SU-8 2050. With the original formulation,
the recommended bake time is ~25 min. at 65 C, followed by ~ 70 min at 95C. Even
if you are using SU-8 2050, the recommended bake is 5 min at 65C, followed by
~45 min at 95C.

SU-8 has a low glass transition temperature (Tg) of 55 C, so if a sufficient
bake is performed, there should be no reason for the film to remain wrinkled
afterwards, since the material should be able to reflow into a highly uniform
coating.


Best Regards,

Chad Brubaker

EV Group       invent * innovate * implement
Technology - Tel: (602) 437-9492, Fax: (602)437-9435 e-mail:
[email protected], www.EVGroup.com

This message and any attachments contain confidential or privileged information,
which is intended for the named addressee(s) only. If you have received it in
error, please notify the sender immediately and then delete this e-mail. Please
note that unauthorized review, copying, disclosing, distributing or otherwise
making use of the information is strictly prohibited.


 -----Original Message-----
From:   [email protected] [mailto:mems-talk-
[email protected]]  On Behalf Of [email protected]
Sent:   Thursday, December 11, 2003 8:26 PM
To:     [email protected]
Subject:        [mems-talk] SU-8 50 wrinkling issue

Dear all,
i am using SU-8 25 to fabricate a 27 micron feature on a 3 inch
glass wafer (Ti seed layer).After the completion of this process, i am
fabricating a 200 microns thick channel as a second layer using SU-8
50.The process parameters for the 200 microns are the following:
200 process parameters (7ml SU-8 50)

?
Spin: 500rpm for 10sec (100rpm/s ramp)
    1500rpm for 30 sec (300rpm/s ramp)
i.e 500.100.10 and 1500.300.30

?
Leave for 1 min

?
Prebake : 65C for 6 minutes and 95C for 22 minutes
?
Exposure: 160microJ/cm2
?
Postbake: 2min at 65C and 95C for 7 minutes
?
Development: 8-10 min with EC Solvent, Clean with IPA afterwards

The problem is that during the prebake phase,the su-8 wrinkles
irreversibly.as a result the structures are very rough
I would very much appreciate any help and/or recommendations on this
problem.Thank you in advance for your help.I am looking forward to your
reply.


________________________________________________________________

DISCLAIMER:

This e-mail and any files transmitted with it are confidential
and intended solely for the use of the individual or entity to
whom it is addressed.  If you are not the intended recipient
you are prohibited from using any of the information contained
in this e-mail.  In such a case, please destroy all copies in
your possession and notify the sender by reply e-mail.  Heriot
Watt University does not accept liability or responsibility
for changes made to this e-mail after it was sent, or for
viruses transmitted through this e-mail.  Opinions, comments,
conclusions and other information in this e-mail that do not
relate to the official business of Heriot Watt University are
not endorsed by it.
________________________________________________________________

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
The Branford Group
Mentor Graphics Corporation
Nano-Master, Inc.