MEMSnet Home: MEMS-Talk: Aluminum evaporation issues
Aluminum evaporation issues
2004-01-07
Sachin Rane
2004-01-07
Steven F. Nagle
2004-01-08
???
2004-01-13
David Grove
2004-01-08
[email protected]
2004-01-13
Sachin Rane
Aluminum evaporation or Aluminum sparker
2004-01-14
hengcw
2004-01-14
R. Brent Garber (2 parts)
2004-01-16
hengcw
Aluminum evaporation issues
???
2004-01-08
"Heat" is the reason for your Aluminum films color is white. reducing the
heat effect as you can.

----- Original Message -----
From: "Sachin Rane" 
To: 
Sent: Thursday, January 08, 2004 1:44 AM
Subject: [mems-talk] Aluminum evaporation issues


> Hi,
> I have been trying to make ~ 1-2 micron thick aluminum films by thermal
> evaporation. The films I get are typically white in color (non-shiny)
> and rough (inspected through AFM). I have used both the boron nitride
> crucible and tungsten boat as the source. The pressure at evaporation is
> typically 2*10^-6 (before starting evaporation it is < 10^-6 ) What is
> the problem? Or is thermal evaporation not a good method for this?
> Thanks
> SR
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
>
>



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Nano-Master, Inc.
MEMS Technology Review
Tanner EDA by Mentor Graphics