A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: thick photoresist development
thick photoresist development
2004-02-16
Qing Yao
2004-02-16
Isaac Wing Tak Chan
2004-02-16
[email protected]
2004-02-16
[email protected]
2004-02-17
Gary
2004-02-17
Brubaker Chad
2004-02-17
Kevin
2004-02-18
Brubaker Chad
2004-02-18
Bill Moffat
thick photoresist development
Isaac Wing Tak Chan
2004-02-16
Hi Qing,

I also had bubbling issue before when I used a similar type of thick film
resist. I found that it is probably due to insufficient softbake time to
remove a large amount of solvent from the spin-coated resist, especially
your film is so thick. Those bubbles are mostly due to N2 evolution during
optical exposure. Can you try increasing the softbake time to 3 mins or
more for each successive bake? It may help. For the resist profile, are
you doing exposure in proximity mode or vacuum contact mode? Gap between
the mask and the wafer is definitely a great cause of the profile shape
and angle. Vacuum contact is much better in make vertical profiles but
defect generation can be a practical issue. Emulsion mask may also have
difficulties in achieving highly vertical profile because of its material
nature. Chrome mask is good for that purpose. Other development modalities
such as puddle development, instead of immersion development, may get more
vertical profile as well.


Yours sincerely,

Isaac Chan

Ph.D. Candidate
Dept. Electrical & Computer Engineering
University of Waterloo
200 University Ave. W
Waterloo, Ontario, Canada
N2L 3G1
Tel: (519) 888-4567, ext. 6014
Fax: (519) 746-6321
[email protected]
http://www.ece.uwaterloo.ca/~a-sidic


On Mon, 16 Feb 2004, Qing Yao wrote:

> Hi,
>
> I have difficulty in patterning thick photoresist. The following is what I
did:
>
> 1> coat a 4" Si wafer with 5 layers of AZ4620 using a spinner. The thickness
of each layer is about 10 microns and the total thickness of PR is about 50
microns. Bake the wafer at 110 degree centigrade for 1 min. after the deposition
of each single layer.
>
> 2> print the image pattern on a transparency (emulsion down) using a 5080-dpi
laser printer. put the transparency mask on top of the PR layer and put a 4"
quartz plate on top of the mask. Then do Fusion Flood exposure. the dose is
about 3300 mJ/cm2. Lots of bubbles are generated during the exposure process.
>
> 3> use 1:4 AZ400K to develop the PR for about 9 minutes.
>
> I used both optical microscope and surface profilometer to measure the side
wall. The slope angle is about 50 degrees.
>
> However, I need the slope angle to be close to 90 degrees (at least larger
than 80 degrees) so that it is almost perpendicular to the substrate. What can I
do to achieve it? Would you please give me any suggestions?
>
> by the way, the thick photoresist layer is sort of mold (for electroless
plating of Ni on Si substrate).
>
>
>
>
> Best Regards,
>
>
> Qing Yao
> ___________________
> M&IE @ UIUC
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
>



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Tanner EDA by Mentor Graphics
University Wafer
Process Variations in Microsystems Manufacturing