Hi Lijun,
  I've tried to make a similar structure with a released membrane size
of 7mm x 7mm out of 2 micron thick LPCVD nitride and ran into the same
problem. That is you end up with a big silicon island in the center that
causes the membrane to break. Our solution was to just DRIE from the
back. If this is not an option for you, you might consider doing a
partial isotropic etch from the back then do the anisotropic etch to
remove the silicon island.

Good luck,
   Mike Martin

>>> [email protected] 03/24/04 1:40 PM >>>
Dear all:

I want to make a large and thin membrane of SC-Si by
KOH etching a SOI wafer. The dimension of the membrane
is about 5mmx5mm square. The SOI wafer has 350nm Si
layer + 1um buried oxide. I use 100nm LPCVD SiN as
protective layer on both side. I etched from backside
with square pattern of 5mmx5mm in SiN. I hope that the
1um buried oxide will act as a stop layer. So finally
I will get a membrane with 100nm SiN + 350nm Si + 1um
SiO2, of 5mmx5mm size, supported by bulk SOI
substrate.

Now I have several questions:

1st, is the membrane of such aspect ratio too fragile
that the stress in it will cause it broken? in other
word, is there anybody have made structure like this?

2nd, it seems that the Si at the edge of the square
etched much faster than in the middle, so it reaches
the buried SiO2 earlier. as a result, I got a
structure of a Si pyramid suspended with thin SiO2+Si
membrane, it broken by itself. also the stress at the
edge seems to cause the SiO2 etch very fast. It lost
the function as a stop layer.

Any comment is welcome and appreciated.

Lijun

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Mentor Graphics Corporation
MEMS Technology Review
University Wafer