Dry etching GaAs
2004-04-23
Greg Chance
2004-04-26
Brent Garber (2 parts)
Dry etching GaAs
Brent Garber
2004-04-26
Dear Gregg,

Here are a few tips for etching GaAs:

Stop with the HCl.  It makes the wafer rough and I don't see your purpose for
needing this step.
Use more Ar that Cl2.
If you don't have a real reason for the silicon or quartz, get rid of them.
Wafer temp is very important.
The hotter your sample gets the faster it will etch
Cl2 seems to always leave me with a rough finish.  I switched to BCl3 (2 sccm)
Ar (8 sccm) @ 20 watts RIE only.  This is much slower, but very smooth.

Brent


Greg Chance wrote:

> Dear all
>
> I'm having a lot of trouble with the dry etching GaAs. Using a CL2 @ 15
> sccm, Ar @ 4 sccm, 4 mTorr pressure, Power RF @ 200W, ICP @ 200W, and a
> de-oxidised silicon wafer on a quartz platter. The surface is very rough
> and etch rate seems to diminish with etch time. The GaAs is de-oxidised in
> HCl and were using Ti as a mask (600nm) for the etch. I need to etch about
> 30um.
>
> Any suggestions?
>
> Regards
> Greg Chance
> Physics Department
> Bath University UK
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
garber.vcf (text/x-vcard, 344 bytes)
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Harrick Plasma, Inc.
MEMS Technology Review
Process Variations in Microsystems Manufacturing