MEMSnet Home: MEMS-Talk: Problem in Lift-off process...
Problem in Lift-off process...
2004-06-28
VELHA Philippe 054082
2004-06-29
hare krishna
Problem in Lift-off process...
VELHA Philippe 054082
2004-06-28
I also do lift off process on no-doped GaN but I think it should be the same
thing.
To answer your question, I think you don't put enought resist on the sample
before spin coating.
I had the same problem, there is resist only on the center of the sample.
If you have tiny samples, like me ( 5mm*5mm)
Try to do that : put your sample on something else like a glass wafer or a
silicon one or something else just to stick on it.
use your resist as a glue, post baking some second.
Spin coat, but put enought resist to overcover your sample and a part of
your support wafer.
It's not sure it works but I do that and the lift off works
An other thing, be sure of the thickness of the resist layer
PS: for information my procedure is
1) cleaning wafer like you
2)spin coating a positive photoresist (S1818) at 3000 rpm for 10s
3) post bake for 2 min at 110°C
4) exposure
5)develop with MF 319 30s


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing
The Branford Group
MEMS Technology Review