Hi ?,

TiO2 is easily etched in CHF3 or SF6 plasmas. The large bias voltage when
using CHF3 usually requires a hard metal mask (tungsten, molybdenum, ...)
and is not applicable to PR. With SF6 I reached selectivities larger than
10:1 using postive PR on sputtered TiO2.

Greetings,

Stefan.





王孝忠 
Gesendet von: [email protected]
08.09.2004 05:58
Bitte antworten an General MEMS discussion


        An:     
        Kopie:
        Thema:  [mems-talk] Dry etch TiO2


Hi.

Does anybody know how do  dry etch TiO2? I use PR as hard mask. But if I
use CF4+O2, the PR will be etched faster than TiO2, besides the etch rate
of TiO2 is much slower. How can I raise the etch rate?

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
Nano-Master, Inc.
The Branford Group
Process Variations in Microsystems Manufacturing