2004-09-17
Do NOT use sputtering for liftoff--especially you are using only 1 layer of
PMMA.  It will make the problem worse due to more isotropic deposition via
sputtering.

Use a Bilayer PMMA of smaller molecular weight UNDER the 950k PMMA.  The
bottom layer should be 2 - 3x the thickness of the metal you are depositing.



-Bill

-----Original Message-----
From: [email protected]
[mailto:[email protected]]On Behalf Of Lee, Duhyun
Sent: Monday, September 13, 2004 6:33 PM
To: General MEMS discussion
Subject: Re: [mems-talk] pmma lift off problem


1. If you evaporated the Cr with e-beam, the e-beam may affect the PMMA.
2. Or in case of  thermal evaporation, substrate must be cool.
3. You'd better try to use thicker PMMA about 100nm and sputtering process.

hope this helpful...


Lee, Duhyun
========================================
----- Original Message -----
From: "Z. Jiang" 
To: 
Sent: Friday, September 10, 2004 9:22 PM
Subject: [mems-talk] pmma lift off problem


> hi all
>
>  I spin coated 15-20nm 950k PMMA on Si chip, baked at 200c for 2min, made
> some pattern and then evaporated 5nm Cr on top. But when I tried to lift
> off it was very difficult. I used acetone, ultrasonic and even oxygen
> plasma. Finally PMMA was lift off but some part of Cr pattern was damaged.
> I guess that was because ultrasonic destroyed the adhesion between Si and
> Cr. I don't know why the lift off can be so difficult. Is that because Cr
> is high-melting-point metal? Can someone tell me? Many thanks.
>
> Cheers
>
> Jiang
>
>
>


_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
MEMS Technology Review
MEMStaff Inc.
Tanner EDA by Mentor Graphics