MEMSnet Home: MEMS-Talk: Protection Layer for SU-8 Structures
Protection Layer for SU-8 Structures
2005-11-07
Silvan Schmid
2005-11-08
walter
2005-11-08
Peter Svasek
Protection Layer for SU-8 Structures
Peter Svasek
2005-11-08
Hi Silvan,

for this purpose I usually use old, expired AZ-positive resist, e.g. AZ 4533
and I remove it with AZ 400k developer UNDILUTED.
AZ 400k developer normally has to be diluted 4:1 , but undiluted
it will strip even unexposed AZ resists.
This developer ist nothing else than diluted KOH, so it will not attack
SU-8.

Another possible way is to flood expose the AZ-resist and to remove it
with normal developer.

regards
Peter

Silvan Schmid wrote:

> Dear all,
>
> I have SU-8 structures which I need to cover with a photoresist layer
> in order to protect them during the dicing process. The solvent to
> remove the protection layer should not alter the SU-8 (e.g. SU-8 will
> swell in acetone).
> Do you have any experience, which photoresist/developer pair is best
> suited for this task?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics
Nano-Master, Inc.
MEMStaff Inc.