MEMSnet Home: MEMS-Talk: help needed for image reversal photoresist AZ5214 with about 3um thickness
help needed for image reversal photoresist AZ5214 with about 3um thickness
2006-03-24
Yawei Li
help needed for image reversal photoresist AZ5214 with about 3um thickness
2006-03-25
Kamesh
help needed for image reversal photoresist AZ5214 withabout 3um thickness
2006-03-26
Lou Chomas
help needed for image reversal photoresist AZ5214 withabout 3um thickness
2006-03-29
Jesse D Fowler
help needed for image reversal photoresist AZ5214 withabout 3um thickness
2006-03-26
Henderson, Andrew
help needed for image reversal photoresist AZ5214 with about 3um thickness
Yawei Li
2006-03-24
Hello everyone,

I am working on the image reversal photoresist AZ 5214 (about 3um
thick)on 4" Si wafer with undercut profile for metal liftoff.

The recipes I tried are as follows:

HMDS
Spin @ 1000 rpm for 45 sec
prebake 95 degree 60 sec on hotplate
Image exposure   5-40 sec at 8.8mW/cm^2
PEB   115 degree for 1-2min on hotplate
Flood exposure 27-120 sec at 8.8 mW/cm^2
Development in AZ 400K (1:4)

But I could not get the feature clear before the exposed area peel off
even I increase the imagewise exposure dose and PEB.

Does anyone have experience with AZ 5214 for 3um thickness?  Can you
share your recipe with me or give me some suggestion about the recipe?

Thanks,

Yawei

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
MEMS Technology Review
Tanner EDA by Mentor Graphics
MEMStaff Inc.