Etching Silicon
Isaac Chan
2006-09-20
Sharukh, you can take O2 out and use pure CF4. If your mask still can't
withstand it, you can add about 10-20% H2 to CF4. You can also use CHF3
instead. Also, low rf power to reduce mask erosion. Since you are only
etching 50nm Si, etch rate is not much of a concern.

Regards,
Isaac Chan, Ph.D.


On Wed, 20 Sep 2006, l ll wrote:

> I would like to know if you knew about any dry etching techniques which would
help me etch single crystal Silicon (approximately 55 nm) using a thinned out AZ
resist as a mask. We have been experimenting with different gasses and their
combinations in a micro RIE. CF4 and O2 can not be used since the both attack
the AZ resist. We have no provisions in the clean room to use HBr or Chlorine.
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
MEMS Technology Review
Addison Engineering
Harrick Plasma, Inc.