A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: photoresist peeled off together with PDMS
photoresist peeled off together with PDMS
2006-10-05
Bo Bob Huo
2006-10-05
Mike Pinelis
答复: [mems-talk] photoresist peeled off together with PDMS
2006-10-05
jianshi
2006-10-05
Bill Moffat
2006-10-10
Bo Bob Huo
2006-10-11
Gareth Jenkins
AZ 9260
2006-10-11
sebastian wicklein
2006-10-13
Isaac Chan
2006-10-13
Bo Bob Huo
2006-10-13
Mike Pinelis
2006-10-14
huy vo
photoresist peeled off together with PDMS
Bo Bob Huo
2006-10-13
Dear all,

Thanks for the suggestions given by some guys. I put a droplet of
chlorinated silane near the wafer in vaccum jar but the PDMS was
still peeled off together with phtoresist. All the chemicals were
newly purchased and in good state.

Overdeveloping may cause this problem? Does anyone encounter this
problem? And how do you solve it? Thanks.

Bob

---------------------------------
When I peeled off the PDMS, the photoresis was always peeled off
together. The procedure is listed as follow. Please give me some
suggestions about which step might cause this problem.

1. Clean silicon wafer for 5 min using oxygen plasma cleaner.
2. Spin adhesion promoter (HMDS/AP010 or AP020) on wafer at the
speed of 2500 rpm for 30 sec hold 5 sec ramp.
3. Immediately spin photoresist (Shipley 1818) on wafer at the speed
of initial spin=500rpm 125 rpm/sec for 10sec, ramp=3000rpm
600rpm/sec over 5sec, spin=hold at max ramp for 30sec.
4. Soft-bake 3min at 105°C and allow to cool up to 30-50
°C on
hotplate (need 10 min).
5. UV exposure for about 1 min.
6. Develop in 351 develooper for > 1 min.
7. Put ~1mL chlorinated silane (tridecafluoro 1,1,2,2 tetrahydro
octyl)-1-trichlorosilane (Sigma, #448931) in a small glass vial and
put in the vacuum chamber for at least 4hrs.
8. Pour the PDMS on the wafer and remove the air bubbles in vacuum
jar for less than 1.5 hour.
9. Put the wafer in the oven at 70°C for 2-4 hours even to
overnight.
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.
MEMS Technology Review
University Wafer