A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Gold were elctroplating onto the edge of photoresist
Gold were elctroplating onto the edge of photoresist
2006-10-26
胡小东
Gold were elctroplating onto the edge of photoresist
2006-10-26
Adamson, Steve
Gold were elctroplating onto the edge of photoresist
Adamson, Steve
2006-10-26
=20
I'm not sure but I think this is caused by lack of agitation in the
bath. A local current density problem. I have seen this before and it
was very difficult to get rid of the problem. In the end we used ion
milling to knock of these upstanding features. Try agitation and playing
with the plating rate and possibly using robbers in the bath to get a
more even plating.=20

Regards,
=20
Steve Adamson
Market Manager, Asymtek
IMAPS President Elect 2007
=20
760-930-7274 office
760-802-1641 Cell
=20
Hope to see you at the Device Packaging Conference & GBC Spring Meeting
March 18-22, 2007, in Scottsdale, AZ
=20
=20
=20

-----Original Message-----
From: [email protected]
[mailto:[email protected]] On Behalf Of ???
Sent: Wednesday, October 25, 2006 7:39 PM
To: [email protected]
Subject: [mems-talk] Gold were elctroplating onto the edge of
photoresist

=20
Dear All,
   In the past two months, while we did gold elctroplating, there were
two gold "wings" extending from the gold line onto the edge of
photoresist.
   photoresist: AZ1500, 2.5 micron thick.
   gold thickness: 2 micron
   "wing" thickness: 3 to 4 micron
   "wing" width: 10 to 20 micron
   =20
   current density 5.5 mA/cm2
   electoplating time 13min
   PH value: 7
   temperature: 50 degree=20
   Has anyone experinced the same problem? May someone would give me any
useful suggextiongs. Thanks!

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing
MEMStaff Inc.