MEMSnet Home: MEMS-Talk: etching AuSn 80-20
etching AuSn 80-20
2007-02-04
Benyimin Hadad
2007-02-05
David Nemeth
etching AuSn 80-20
David Nemeth
2007-02-05
Te handbook of metal echants, page 610.

They list:
Aqua Regia:
3:1 HCL:HNO3, room temp

You can also use KCN (potassium cyanide), or a Tri iodide etch (400g KI,
200G I2, 1000ml H2O)

-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of Benyimin Hadad
Sent: Sunday, February 04, 2007 5:00 PM
To: General MEMS discussion
Subject: [mems-talk] etching AuSn 80-20

Hello all

I want to etch AuSn 80-20, with wet etching.
How can I etch it?


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
MEMS Technology Review
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing