A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Depositing metals onto plastics and SU-8
Depositing metals onto plastics and SU-8
2007-03-01
Jon Fox
2007-03-01
Brent Garber
2007-03-03
Roger Shile
2007-03-03
Mantavya Sinha
2007-03-03
Kirt Williams
2007-03-01
Mohamad Hajj Hassan
2007-03-02
Samadhan Bhaulal Patil
2007-03-03
[email protected]
2007-03-04
[email protected]
2007-03-05
Jesse D Fowler
2007-03-06
Yue Mun Pun, Jeffrey
Depositing metals onto plastics and SU-8
Mantavya Sinha
2007-03-03
You are right Roger. E-Beam is not going to be a cool process. In my
experience Sputtering should give you near room temperature (RT +
10'C-15'C) deposition.

Cheers

Mantavya Sinha
PhD Student
Dept of ECE
NUS


-----Original Message-----
From: [email protected]
[mailto:[email protected]] On Behalf Of Roger Shile
Sent: 03 March 2007 09:41 AM
To: 'General MEMS discussion'
Subject: RE: [mems-talk] Depositing metals onto plastics and SU-8


Contrary to many postings here, E-beam evaporation is thermal
evaporation; the charge is not cool by any means.

Roger Shile

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
MEMS Technology Review
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing