trupti shantaram khaire
2007-04-23
Ad Hall
2007-04-23
Roger Shile
Nb RIE using SF6
Ad Hall
2007-04-23
Trupti,

What are your process conditions?  Polymer formation is to the square of the
pressure.  Lower pressure = lower polymer.

John Hall


-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of trupti shantaram khaire
Sent: Sunday, April 22, 2007 5:28 PM
To: [email protected]
Subject: [mems-talk] Nb RIE using SF6

Hi,
I am trying to etch Nb with SF6. I noticed that there is lot of polymer
formation on the Si Substrate surrounding my desired Nb feature. I was
thinking of using SF6+O2 to avoid polymer formation. Adding O2 to SF6 means
photoresist will be etched at a greater rate. It also means that polymer
which is most likely acting as a etch stopper for Si will in its absence
cause Si to etch faster, which is even more detrimental because it will end
up in making a big trench next to Nb feature.(I already noticed the Si etch
of 500nm in 4 min)
Any alternative that anybody knows to avoid Si etch?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing
MEMStaff Inc.
MEMS Technology Review