A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: RIE removal of S1818 photoresist
RIE removal of S1818 photoresist
2008-01-16
Curtis, Mark E.
2008-01-16
Bob Henderson
Fluorine residues etching Cr and Au
2008-01-17
Jason Milne
2008-01-17
Bob Henderson
2008-01-18
Martin Lapisa
2008-01-17
Jaibir sharma
RIE removal of S1818 photoresist
Bob Henderson
2008-01-16
Mark:

I was surprised to hear your system etched Cr at all. Do you run other etch
processes in your system using fluorine or chlorine? If so you probably need
to clean the chamber to remove polymers containing residues other than pure
oxygen during ash. Your conditions look reasonable but using more rie power
at lower time might help as the Trion with ICP has been reported to generate
a lot of heat to the substrate or so I have heard. Bob Henderson

----- Original Message -----
From: "Curtis, Mark E." 
To: 
Sent: Wednesday, January 16, 2008 8:44 AM
Subject: [mems-talk] RIE removal of S1818 photoresist


Hello all,

I’m using Shipley S1818 positive photoresist as a mask for wet-etching a
100
nm thick film of chromium.  After using a wet chemical photoresist stripper
there remains some photoresist residue on the surface of the chromium.
I’ve
attempt to use a Trion RIE to remove the photoresist residue with the
following etch parameters:
Gases/Flow Rate (O2/50 sccm),
Pressure (500 mTorr),
RIE Power (25 W), ICP Power (500 W), and
Time (30 min).

To my surprise, I found that not only did it remove the photoresist but also
the chromium.  Does anyone know of a good photoresist removal recipe for RIE
that will not etch chromium.  I have previously tried a shorter etch time
(~10 min) but it did not completely remove the photoresist residue.

Mark E. Curtis
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Addison Engineering
University Wafer
Tanner EDA by Mentor Graphics