Hi all

Several days ago I asked some questions on SU-8 process on PECVD SiO2.
At that moment, my major problem is that SU-8 keeps peeling off from
Si Sub which is covered with PECVD SiO2 during the development, while
the same process on bared Si is no problem. (The reason I still not
very sure)

My way is to get a 5mins O2 plasma treatment on sample, and all the
baking sections (65-95C) use ramping rather than change the
temperature immediately. For my case, SU-8 2050
1)  O2 plasma 100w 5 mins on Sub
2)  Dehydrate 200C for 15mins
3)  Spin coat SU-8 2050 at 4000rpm
4)  Softbake: 65C 10mins, 95C 20 mins (ramping, and cool to room temperature-RT)
5)  Exposure 45s at 7mW/cm2
6)  PEB: RT to 65C stay for 10mins, ramp to 95C stay for another
30mins and cool to RT
7)  Develop 3 mins with rinse in IPA
8)  Hardbake: RT to 150C stay for 15 mins

Hope this recipe could help you out of such SU-8 problem which I
suffered in the last several weeks. and if anyone know the reason why
the different performance happens on PECVD SiO2 and bare Si (with
native oxide layer), I appreciate your sharing to us!

Thanks and good luck!

Steven
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
MEMStaff Inc.
Harrick Plasma, Inc.
University Wafer