MEMSnet Home: MEMS-Talk: Hydrophobic treatments/coatings for Polycarbonate
Hydrophobic treatments/coatings for Polycarbonate
2008-04-09
Paul Monaghan
2008-04-09
Adrian Brozell
2008-04-09
Paul Monaghan
2008-04-09
Boris Kobrin
2008-04-10
Paul Monaghan
Hydrophobic treatments/coatings for Polycarbonate
Paul Monaghan
2008-04-10
Hi Boris,

Thanks for the information. This sounds interesting, as does using Teflon AF
described by Kevin Tsao. 112-115deg is right in in ball park of contact angles
I am after.

Is your method proprietary? If not, can it be adapted using standard (and
simple if possible!) lab methods? Is it possible you could forward some further
details or alternatively point me in the right direction?

Many thanks and best regards,

Paul

Quoting Boris Kobrin :

> Hi Paul,
>
> You can use simple vapor deposition method to change wettability of your
> polycarbonate. We usually getting 112-115 deg DI water contact angle on
> polycarbonate samples (depends on initial surface roughness). In-situ (vapor
> deposited) adhesion layer should be used in order to attach self-assembled
> hydrophobic monolayer to polymer materials, though total thickness of the
> dual layer can be kept below 100 A and the entire process is automated.
>
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Nano-Master, Inc.
Tanner EDA by Mentor Graphics
Harrick Plasma, Inc.