MEMSnet Home: MEMS-Talk: Effect of EDP/KOH on PDMS andphotopatternable silicone
Effect of EDP/KOH on PDMS and photopatternable silicone
2008-07-17
Anurag Tripathi
Effect of EDP/KOH on PDMS and photopatternable silicone
2008-07-19
shay kaplan
Effect of EDP/KOH on PDMS andphotopatternable silicone
2008-07-21
Roger Shile
Effect of EDP/KOH on PDMS andphotopatternable silicone
Roger Shile
2008-07-21
I wonder if a PDMS bond between two wafers will withstand a KOH etch, or
will the interface fail?

Roger Shile

-----Original Message-----
KOH doesn't affect PDMS
Shay
-----Original Message-----

Hello,

I wanted to know if anyone of you has an experience with performing
EDP/KOH etch of a Si wafer with PDMS or photopatternable silicone WL
5150 patterned on the back side. Does the EDP/KOH etch damage the PDMS
or the photopatternable silicone?

Thank you very much,

Anurag Tripathi
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Addison Engineering
Harrick Plasma, Inc.
University Wafer