A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Su 8 thickness
Su 8 thickness
2008-08-06
jiang Liudi
2008-08-06
Wei Cheng
2008-08-07
jiang Liudi
2008-08-08
eowin rohan
2008-08-06
jiang Liudi
2008-08-06
Oakes Garrett
2008-08-07
jiang Liudi
2008-08-08
Oakes Garrett
2008-08-12
jiang Liudi
2008-08-13
Oakes Garrett
Su 8 thickness
Oakes Garrett
2008-08-06
Try using more resist and slowing down the spin speed.  Alternatively, use a
double coat process.  I have had much success with a double coat process to 500
µm using SU-8 2100.

Best Regards,
Garrett Oakes

EV Group
invent * innovate * implement
Regional Sales Manager North America - Direct: +1 (480) 305 2443, Main: +1 (480)
305 2400 Fax: +1 (480) 305 2401
Cell: +1 (480) 516 6724
E-Mail: [email protected], Web: www.EVGroup.com

-----Original Message-----
From: jiang Liudi [mailto:[email protected]]
Sent: Wednesday, August 06, 2008 5:51 AM
To: [email protected]
Subject: [mems-talk] Su 8 thickness

Dear all,

I was trying to obtain >100um thick of patterned SU8 2075. The used receipe is
as follows:

spin: 500rpm/10s+1700rpm/30sec
soft bake: 65 C/5 mins +95 C/20min
UV expose: 28 sec.
PEB: 65 C/5 mins +95 C/10 min
develop: 10 mins.

all designed patterns are large ( all around 50-200um). However, using profiler,
the  step of the developed patterns is only about 66 um thick.

Could anyone kindly suggest the possible reasons for such thin resist?

Many thanks.
Jiang

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
Harrick Plasma, Inc.