A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: SU-8 delamination problem
SU-8 delamination problem
2008-10-23
Dhananjay Dendukuri
2008-10-23
Bruce Altemus
2008-10-23
Gareth Jenkins
2008-10-23
Eric Johnston
2008-10-23
Jian Wang
2008-10-23
Bill Moffat
2008-10-24
Meifang Lai
2008-10-24
Gareth Jenkins
2008-10-25
Dendukuri
2008-10-23
Michael Larsson
SU-8 delamination problem
Bruce Altemus
2008-10-23
Dhananjay,

The cause of your issue is most likely a humidity one. I would suggest
performing a dehydration bake after your piranha clean. This should
resolve your issue...

Good luck.

Regards,
Bruce


________________________________

From: [email protected] on behalf of Dhananjay Dendukuri
Sent: Thu 2008.10.23 02:18
To: [email protected]
Subject: [mems-talk] SU-8 delamination problem


Dear all,

I have a severe problem of SU8 delamination. Please go through my
process below and advise

I am fabricating an array of 100 microchannels of 50 micron width and 40
micron depth (the gap between two channels is 100 micron) on a 4 inch
silicon wafer using *Su8 2035* negative resist. The process flow is
given below.

1. Hard bake - 150 C for 20 min (after cleaning silicon wafer in Piranha
solution).
2. Spin coat - 15 sec at 400 rpm followed by 30 sec at 2000 rpm.
3. Soft bake - 3 min at 65 C and 5 min at 95 C. (wait for 10 min)
4. UV expose - 28 sec to get an exposure energy of 220 mJ/cm2.
5. PEB - 30 min at lower initial temperature of 65 C and ramping up the
temperature to 95 C in every 15 min with every 10 C increase. (Wait for 10
min)
6. Development - In ultrasonic bath (without sonicator SU8 in the channel
path is not possible to remove completely).

Within 1 min of development, all the channels are completely
delaminated.  We
tried the process on many wafers by changing different soft bake and PEB
timings, but nothing is working.  Any suggestions to avoid delamination
problem are deeply appreciated.

Thank you

Dhananjay
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Harrick Plasma, Inc.
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing