very thick layer of SU-8
2008-11-26
A. AhmadShukri
2008-11-26
Bill Moffat
2008-11-26
John Hilton
2008-11-27
郑瑞麟(Ruilin Zheng)
2008-11-27
Gareth Jenkins
2008-11-27
Liang Zhao
2008-11-27
Michael Riss
2008-12-01
Oakes Garrett
2008-12-02
Shao Guocheng
2008-12-02
Gareth Jenkins
2008-12-02
Jacques Jonsmann
2008-12-03
郑瑞麟(Ruilin Zheng)
2008-12-03
Shao Guocheng
2008-12-03
Oakes Garrett
very thick layer of SU-8
郑瑞麟(Ruilin Zheng)
2008-12-03
Hello, Guocheng,

I experienced what you call wrinkles during post exposure bake, and my
structures were also distorted.

I think this are caused by the severe stress during soft-bake and exposure,
especially for ultra thick layer.

pls try to lower your baking temperature for both soft and post bake, and
greatly extend your baking time at lower temperature. That may help you
solve the wrinkles.

Good luck!

On Tue, Dec 2, 2008 at 10:19 AM, Shao Guocheng  wrote:

> Hi, All:
>
>    So what kinda softbaking process u guys using for ultra-thick SU-8
> layer. I'm working with 1mm thick SU-8. My process is:
>
> Spincoating first layer(around 500um), softbake at 65C for about 2 hours
> and slowly ramp to 110c, hold for 6 hours and slowly ramp to room temp. for
> the first layer I can bake out aroun 28% of the solvent which SU-8 50 should
> have 31%. But the remaining 3% seems not a big problem and I can finish my
> first layer exposure pretty well.
>
> for the second layer, I use almost the same process, but hold at 110c for
> 8hr, but I can only bake out around 24% of solvent. Because of that, during
> my PEB process, severe wrinkle happen around 50-60C, although it will smooth
> out after a while, some of my fine structures r destorted by these wrinkles.
> I tried to lower the baking temperature to 90C and bake for 15hrs, but
> still, only 24%-25% of solvent can be bake out.
>
> Any one has a cure for this prolem? thx a lot
>
> Guocheng Shao

--
Best Regards,

郑瑞麟

Ruilin Zheng

Address:
Pen-Tung Sah MEMS Research Center,
Xiamen University, Xiamen,361005,
P.R.China
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
MEMStaff Inc.
Nano-Master, Inc.
University Wafer