MEMSnet Home: MEMS-Talk: glass cracking during anodic bonding
glass cracking during anodic bonding
2009-02-26
jingru zhang
2009-02-26
Mehmet Aykol
2009-02-26
jingru zhang
2009-02-27
shay kaplan
2009-02-27
jingru zhang
2009-02-28
shay kaplan
2009-02-27
Staller, Steven E
2009-02-27
jingru zhang
2009-02-27
Brad Johnson
2009-02-27
jingru zhang
2009-03-02
Brad Johnson
2009-03-03
jingru zhang
2009-03-04
Brad Johnson
glass cracking during anodic bonding
Brad Johnson
2009-02-27
Hello Jingru,

There are many things that can cause the cracking.  What do the cracks look
like?  Are they round cracks or half moon cracks?  What type of bonder are you
using, homemade hotplate and power supply or a commercial chamber bonder?  Are
you bonding in vacuum or atmosphere?

If you are seeing half moon cracks or round chunks of glass popping out then you
have air (or gas) getting trapped between two bond fronts.  The gas will be
compressed until it cracks the glass and vents.  If you have long cracks the
follow your channels then the trapped gas in the channels may be cracking the
glass, I've never seen this case but it could be an issue.

Try this:
1.  If you are using a chamber bonder make sure it is setup properly and the
upper and lower electrodes are clean and flat.  Metal electrodes tend to warp
and pit over time.  If this is the case then it will cause poor contact with the
bond stack and allow air or gas to become trapped.  SiC electrodes will become
contaminated with Na after several bonds.  Give them a good clean in RCA over
night and the conductivity should be back to new and uniform across the chuck.

2.  Try bonding in a vacuum or at a lower pressure.  If you bond at a low
pressure make sure it is below 1e-2mbar or you risk the chance of generating a
plasma in the chamber.  You'll know if you have a plasma because the current
will stop dropping and the voltage will stop increasing and stay and a constant
state.

3.  If you cannot bond in a vacuum and trapped gas is the issue the try bonding
at a lower current.  This will slow the bond front and may help to allow the gas
to vent before it gets trapped in the bond.

4.  If the cracking is general cracks across the wafer check your ramping and
cooling times.  Let the wafer stack slowly heat up then let them set at the
bonding temp to come to a nice uniform temp before bonding.  Any time I set up a
first time bond I let the wafers ramp up to 350C over a 30 minute time.  Then I
will heat to 400 and hold for 15 minutes to allow the tool and the wafer stack
to stabilize.  After bonding I remove any force on the stack and cool the wafers
slowly at about 100C over a 30 minute time.  If you have the ability to apply
force do not heat or cool the stack with force, this can not only cause a shift
in the wafer stack but also cause cracking..  This sounds like a very long
recipe but once you have a working process you can optimize it for throughput.

Good Luck

Brad Johnson
Application Engineer
DJK Global
US Distributor, Semiconductor Inspection Systems
2447 W. 12th St. - Suite 6, Tempe, AZ 85281
480-968-3343 Ext 112 office
602-501-4413 cell
[email protected]
http://www.djksemi.com



-----Original Message-----
From: jingru zhang [mailto:[email protected]]
Sent: Thursday, February 26, 2009 9:12 AM
To: [email protected]
Subject: [mems-talk] glass cracking during anodic bonding

Dear all,

I have deep channels (around a hundred microns) on the silicon substrate. and
during the anodic bonding of silicon and glass, they bonded well but the
glass cracked. Maybe it is the stress around the channels walls which caused
cracking. The voltage I am using now is 500 w, and the temperature goes to
400 deg c.  Does anyone have similar experience? How to avoid this?

Thank you very much.

Best Regards,
Jingru

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
MEMStaff Inc.
MEMS Technology Review
University Wafer