A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: metallic mask
metallic mask
2010-04-02
Andrea Mazzolari
2010-04-05
Ruiz, Marcos Daniel (SENCOE)
2010-04-28
Micro Fab
2010-04-05
Andrea Mazzolari
2010-04-05
Ruiz, Marcos Daniel (SENCOE)
metallic mask
Ruiz, Marcos Daniel (SENCOE)
2010-04-05
Andrea,

I've found that the biggest challenge when using evaporated metal this
way is particles.  Every particle results in a pinhole in your mask that
allows the etchant to get under the mask.

Dan

-----Original Message-----
From: mems-talk-bounces+dan.ruiz=honeywell.com@memsnet.org
[mailto:mems-talk-bounces+dan.ruiz=honeywell.com@memsnet.org] On Behalf
Of Andrea Mazzolari
Sent: Friday, April 02, 2010 10:41 AM
To: mems-talk@memsnet.org
Subject: [mems-talk] metallic mask

Hi all,

i need to thermal evaporate a metallic mask on a polished silicon wafer.
The mask should withstand 40% KOH etch for 5 hours.
I tried 20/30 Cr/Au, but it seams that it is not working: after about 1
hour etch many pinholes are generated in the Cr/Au layer, KOH penetrates
such pinholes and etch silicon.

Any suggestion on how to improve the resistance of Cr/Au layer ?
Any alternative to Cr/Au ?

Thanks,
Andrea
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
The Branford Group
Harrick Plasma, Inc.
MEMStaff Inc.