A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Removing hard-baked photoresist
Removing hard-baked photoresist
2010-06-22
ameya g
2010-06-23
antwi nimo
2010-06-23
Jesse D Fowler
2010-06-24
Jie Zou
2010-06-24
Morrison, Richard H., Jr.
2010-06-25
[email protected]
2010-06-24
Mike Whitson
2010-06-24
Bill Moffat
2010-06-24
Michael D Martin
2010-06-25
ameya g
Removing hard-baked photoresist
Jesse D Fowler
2010-06-23
Piranha (in my case 4:1 H2SO4 : 30%H2O2) boils at 160C. It is much more
aggressive at this temperature. (also very dangerous!)


----- original message ----
From: antwi nimo 
To: [email protected], General MEMS discussion 
Date: 06/23/2010 09:47 AM
Subject: Re: [mems-talk] Removing hard-baked photoresist


A mixture of H2SO4 and H2O2 at a temperature of  ~180celsius can remove
the resist...This solution is used the remove resist when making glass
mask...I am sure it can remove this resist to.....i hope this information
helps,
Nimo


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Addison Engineering
Mentor Graphics Corporation
University Wafer