A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Recipe of Ar plasma etching gold
Recipe of Ar plasma etching gold
2011-10-12
Yingtao Tian
2011-10-12
Bill Moffat
2011-10-12
Matthieu Nannini, Dr.
2011-10-12
志修 梁
2011-10-12
Yingtao Tian
2011-10-13
Kirt Williams
2011-10-30
Khaled Mohamed Ramadan
2011-10-31
Kirt Williams
Recipe of Ar plasma etching gold
Kirt Williams
2011-10-13
I've stripped off thin Au/Cr before with argon in an ion mill at 500 V and ~1
mA/cm2. You should be able to get something similar with a parallel-plate plasma
setup. I'd start with high power, which yields a high voltage. Also, use a low
argon pressure (say 2 mTorr), which makes the voltage higher and the current
lower for a constant power.

   --Kirt Williams

-----Original Message-----
From: [email protected] [mailto:mems-
[email protected]] On Behalf Of Yingtao Tian
Sent: Wednesday, October 12, 2011 1:49 PM
To: 志修 梁; General MEMSdiscussion
Subject: Re: [mems-talk] Recipe of Ar plasma etching gold

Hi,

Thank you guys for replying. Actually, when I asked 'etching', I did mean the
plasma sputter off material. Because I have other components on some area of the
wafer, the wet etching process can damage my components. So, I am thinking an
inert Ar plasma may be better choice to remove the 100nm Au and Cr.

If any of you could give me something to start with, then I may be able to work
out my own parameters more quickly.

Thanks again.

Yingtao
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
Addison Engineering
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics