MEMSnet Home: MEMS-Talk: silicon KOH etch
silicon KOH etch
2012-03-01
Xing Sheng
2012-03-01
Roger Shile
2012-03-02
Xing Sheng
2012-03-02
Kirt Williams
silicon KOH etch
Kirt Williams
2012-03-02
Xing:
Note that the flat on a silicon wafer is  a <110> direction, not a <100>
direction, so the sides of your pits should be parallel and perpendicular to
the flat. Maybe that's the source of the confusion. The surface of an (001)
wafer points in the [001] direction.
   --Kirt Williams

-----Original Message-----
From: [email protected] [mailto:[email protected]]
On Behalf Of Xing Sheng
Sent: Thursday, March 01, 2012 4:30 PM
To: mems-talk
Subject: Re: [mems-talk] silicon KOH etch

That was what I expected. However, I still get a pit of size d^2 along 100
direction, and the facet angle is almost 55 degree. So I get confused...

------------------
Best regards,

Xing Sheng

2012-03-01



From: Roger Shile
Date: 2012-03-01 15:49
To: General MEMS discussion
Subject: Re: [mems-talk] silicon KOH etch Any shape of mask opening will
eventually etch to a pyramidal pit bounded by 111 planes.  The orientation
of this pit is fixed.  The size is determined by the extent of the mask
opening in the 110 directions.
A square opening with side length d aligned to the 100 direction will result
in a pyramidal pit with a base dimension d*sqrt2.  (a square circumscribed
on the original square at 45 degrees).

Roger Shile



From: [email protected]
[mailto:[email protected]] On Behalf Of Xing Sheng
Sent: Wednesday, February 29, 2012 3:20 PM
To: mems-talk
Subject: [mems-talk] silicon KOH etch



Hi,



I have a question about 100 silicon wafer KOH anisotropic etch.



I opened a square window on 100 silicon using SiN as protection.
Normally the window should be aligned along 110 direction, so that we can
get inverted pyramid structure, and the plane angle is 55 degree.
However, I opened the window along 100 direction. It seems similar pyramid
is obtained. This is weird. What is the plane direction I got, and what is
the side wall angle at this time?



Thanks!



------------------

Best regards,

Xing Sheng

2012-02-29

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Mentor Graphics Corporation
University Wafer
Tanner EDA by Mentor Graphics