AZ5218 PR issue in Metal Lift off process
2013-02-01
Wei Cheng
2013-02-04
shay kaplan
AZ5218 PR issue in Metal Lift off process
shay kaplan
2013-02-04
Nitrogen is released when the resist is exposed. If your rather high temp
softbake creates a crust on the resist surfaces, the nitrogen might not have
a way to escape.
You might want to reduce the SB temp to 95 deg.

-----Original Message-----
From: [email protected]
[mailto:[email protected]] On Behalf Of Wei Cheng
Sent: Friday, February 01, 2013 6:25 AM
To: General MEMS discussion
Subject: [mems-talk] AZ5218 PR issue in Metal Lift off process


I use AZ5218 in metal lift off process. I have seen lots of bubbles in the
PR sometimes. See pictures below. Lots of bubbles form a line in the center
of the scribe-line. The bubble line lies at exactly where two exposure
fields overlap. So the PR in this 10um width strip sees double exposure. And
this strip is where I can find most of the bubbles. This bubble issue does
not happen always. On some other wafers or even some other portion of the
same wafer, I can only find much less bubble.

One time I did inspection right after post exposure bake (PEB) I saw the
bubbles on the wafer already.


This is a mystery to me. Anyone has any idea what could be wrong?


Spin speed of ~1000rpm=20

Soft bake: 110C/90"=20

~3.7um film thickness

Exposure: 55~70mj in Canon i1 stepper

PEB: 115C / 75"~90"

Flood exposure 300" in Quintel aligner

Develop: diluted AZ400K / 100"

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing
MEMStaff Inc.
Harrick Plasma, Inc.