A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Improving adhesion of sputtered metals on borofloat glass
Improving adhesion of sputtered metals on borofloat glass
2015-06-30
Gianmario Scotti
Improving adhesion of sputtered metals on borofloat glass
2015-06-30
[email protected]
2015-07-01
Ruiz, Dan (SGNCOE)
2015-07-01
André Bödecker
2015-07-01
Gianmario Scotti
Improving adhesion of sputtered metals on borofloat glass
2015-07-01
shay
Improving adhesion of sputtered metals on borofloat glass
Gianmario Scotti
2015-07-01
Hello Andrè,


I was planning on doing an oxygen plasma cleaning step. Thank you for
confirming that this idea might help.


mario

On Wed, Jul 1, 2015 at 7:58 AM, André Bödecker <
[email protected]> wrote:

> Hello Mario,
>
> a good cleaning step can improve the adhesion of sputtered layers,
> especially on borofloat wafers.
>
> Regards,
> André Bödecker
>
> -----Ursprüngliche Nachricht-----
> Von: [email protected]
> [mailto:[email protected]] Im
> Auftrag von [email protected]
> Gesendet: Dienstag, 30. Juni 2015 22:59
> An: General MEMS discussion
> Betreff: Re: [mems-talk] Improving adhesion of sputtered metals on
> borofloat
> glass
>
> Hi Mario,
>    Nickle is a great adhesion layer, though if you are doing
> electrochemistry I would use tantalum.
>
> Regards,
>   Michael
> ________________________________________
> From: [email protected]
> [[email protected]] on behalf of
> Gianmario Scotti [[email protected]]
> Sent: Thursday, June 25, 2015 6:20 AM
> To: General MEMS discussion
> Subject: [mems-talk] Improving adhesion of sputtered metals on borofloat
> glass
>
> Hey all,
>
>
> I am sputtering platinum on borofloat (i.e. "pyrex") glass using ~10 nm of
> chromium as adhesion layer. Adhesion seems poor, and I am looking at
> various
> ways to improve it. Could you suggest some?
>
>
>
> mario
>
>
>
>
>
>
> --
> Gianmario Scotti
>
> Post-doc researcher
> Helsinki University
> Division of Pharmaceutical Chemistry and Technology Viikinkaari 5E (PO Box
> 56) FI-00014
>
> https://urldefense.proofpoint.com/v2/url?u=http-3A__www.helsinki.fi_pharmacy
>
> _chemtech_en_index.html&d=AwICAg&c=SgMrq23dbjbGX6e0ZsSHgEZX6A4IAf1SO3AJ2bNrH
>
> lk&r=iuM4gMLa1Lu9rB1E3CyO_FZKwp19zNE1F2fh6h-VHUI&m=0cmX1qq5gVgqV4OGDFRtap2ne
> AzEcn1KB8cwiSbazk4&s=yESeMzqE9qJoCEKLDfd5aYhSm_UPyOu6xAG37yVtNXA&e=
>
>
> Visiting researcher
> Aalto University, School of Electrical Engineering
>
> https://urldefense.proofpoint.com/v2/url?u=http-3A__elec.aalto.fi_en_&d=AwIC
>
> Ag&c=SgMrq23dbjbGX6e0ZsSHgEZX6A4IAf1SO3AJ2bNrHlk&r=iuM4gMLa1Lu9rB1E3CyO_FZKw
>
> p19zNE1F2fh6h-VHUI&m=0cmX1qq5gVgqV4OGDFRtap2neAzEcn1KB8cwiSbazk4&s=UA0xV_exl
> Jz7ciI-2auMWZP11lFLz5CIJVEeoqzHOtw&e=
> <
> https://urldefense.proofpoint.com/v2/url?u=http-3A__materials.aalto.fi_en_&
>
> d=AwICAg&c=SgMrq23dbjbGX6e0ZsSHgEZX6A4IAf1SO3AJ2bNrHlk&r=iuM4gMLa1Lu9rB1E3Cy
>
> O_FZKwp19zNE1F2fh6h-VHUI&m=0cmX1qq5gVgqV4OGDFRtap2neAzEcn1KB8cwiSbazk4&s=Kkz
> AjNpTW7rhHC-HuELMMgMGQMi8Myv_OcbtbhI8tnw&e= >
>
> Micronova, Tietotie 3
> 02150 Espoo
> Finland
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at
>
> https://urldefense.proofpoint.com/v2/url?u=http-3A__www.mems-2Dexchange.org&
>
> d=AwICAg&c=SgMrq23dbjbGX6e0ZsSHgEZX6A4IAf1SO3AJ2bNrHlk&r=iuM4gMLa1Lu9rB1E3Cy
>
> O_FZKwp19zNE1F2fh6h-VHUI&m=0cmX1qq5gVgqV4OGDFRtap2neAzEcn1KB8cwiSbazk4&s=l7e
> g-UW7G2-CZ0z6xpz4BbB8r4PNavvUSnDABa33Nd0&e=
>
> Want to advertise to this community?  See
>
> https://urldefense.proofpoint.com/v2/url?u=http-3A__www.memsnet.org&d=AwICAg
>
> &c=SgMrq23dbjbGX6e0ZsSHgEZX6A4IAf1SO3AJ2bNrHlk&r=iuM4gMLa1Lu9rB1E3CyO_FZKwp1
>
> 9zNE1F2fh6h-VHUI&m=0cmX1qq5gVgqV4OGDFRtap2neAzEcn1KB8cwiSbazk4&s=ALXRzcSqy65
> ZipNkbxDc0hsoJdwqZveMCTQ3vc8iAM8&e=
>
> To unsubscribe:
>
> https://urldefense.proofpoint.com/v2/url?u=http-3A__mail.mems-2Dexchange.org
>
> _mailman_listinfo_mems-2Dtalk&d=AwICAg&c=SgMrq23dbjbGX6e0ZsSHgEZX6A4IAf1SO3A
>
> J2bNrHlk&r=iuM4gMLa1Lu9rB1E3CyO_FZKwp19zNE1F2fh6h-VHUI&m=0cmX1qq5gVgqV4OGDFR
> tap2neAzEcn1KB8cwiSbazk4&s=vas6fhpH1St4XLaNGZMXxuFtBlzg6HiCtF1EubUcPYc&e=
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>



--
Gianmario Scotti

Post-doc researcher
Helsinki University
Division of Pharmaceutical Chemistry and Technology
Viikinkaari 5E (PO Box 56) FI-00014
http://www.helsinki.fi/pharmacy/chemtech/en/index.html


Visiting researcher
Aalto University, School of Electrical Engineering
http://elec.aalto.fi/en/ 

Micronova, Tietotie 3
02150 Espoo
Finland
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search