MEMSnet Home: MEMS-Talk: About difficulty in photoresist development (if using HMDS as adhesion layer)
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-23
Mehmet Yilmaz
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
Bill Moffat
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
André Bödecker
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
James Guenes
2015-09-25
Liang Zhao
2015-09-25
Orozaliev Ajymurat Nurdinovich
2015-09-29
Mehmet Yilmaz
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-25
Mohammad Yusuf Mulla
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-29
Andrew Sarangan
2015-09-30
Mehmet Yilmaz
2015-10-04
Andrew Sarangan
2016-01-04
Mehmet Yilmaz
2016-01-04
조명래
2016-01-04
ozgur celik
2016-01-05
André Bödecker
2015-09-25
Brian Baker
About difficulty in photoresist development (if using HMDS as adhesion layer)
Brian Baker
2015-09-25
Mehmet,



It sounds like you may be using undiluted HMDS which can react with your
photoresist and render it undevelopable.  We usually dilute our HMDS with
Xylene (80:20 Xylene: HMDS) before the dispense/spin cycle.  A 3000 rpm, 60
second spin cycle with the diluted HMDS should leave a layer that will
improve adhesion without affecting the photoresist that is subsequently
spin-coated.



Best,



Brian Baker

Utah Nanofab





_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
MEMS Technology Review
Tanner EDA by Mentor Graphics
Harrick Plasma, Inc.