There are several different Aluminium etchants know. Most of them are based
on Phosphoric Acid 85%(about 60 to 90 parts per volume) and Nitric Acid 70%
(about 2 to 10 parts per volume). Sometimes people add Acetic Acid (about
10-30 parts per volume) for better wetting behaviour and lower viskosity.
Merck Corporation has about 10 different Aluminium etchants.

Best regards

Armin Kuebelbeck
______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
MEMS Technology Review
Addison Engineering
Process Variations in Microsystems Manufacturing