BERAUER,FRANK (HP-Singapore,ex7)
Hard mask for 20 um deep SiO2 RIE etch?
BERAUER,FRANK (HP-Singapore,ex7)
2001-12-20
SU-8 (especially heavily cross-linked films) does not strip well
in Oxygen plasma. Adding Hydrogen radicals helps a lot. We tried
NH3, but other sources, e.g. forming gas, should work as well.

Seasons Greetings,
        Frank Berauer
        Senior R&D Engineer
        Hewlet-Packard Singapore


-----Original Message-----
From: Liz Shelley [mailto:[email protected]]
Sent: 20 December 2001 22:57
To: [email protected]
Subject: Re: [mems-talk] Hard mask for 20 um deep SiO2 RIE etch?


BOB
Can you give me details on the parameters by which you ash SU-8
(Power/gases/flows/processing pressures)?
Thanks for your help
Liz

> From: [email protected]
> Reply-To: [email protected]
> Date: Wed, 19 Dec 2001 16:05:10 EST
> To: [email protected]
> Subject: Re: [mems-talk] Hard mask for 20 um deep SiO2 RIE etch?
>
> We have good results with oxide as a hard mask. Typical selectivities are
>> 60:1 using oxide. Better than that we have had great results using SU-8
from
> Microchem corp. Initial results show a 40:1 selectivity pr:silicon and
SU-8
> formulations can range from 5-100 microns. It also seems to ash or strip
> reasonably well at around 3 microns/minute. Bob Henderson
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.mems-exchange.org/
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Process Variations in Microsystems Manufacturing
Nano-Master, Inc.
Harrick Plasma, Inc.