Kirk,

Try longer softbake time. I'm using it in all MEMS products more than 8
microns. Approx 10 min @ 115 degrees hot plate.

Ha Vu
TRW NovaSnesor

> -----Original Message-----
> From: kirt_williams@agilent.com [SMTP:kirt_williams@agilent.com]
> Sent: Wednesday, January 16, 2002 2:56 PM
> To:   mems-talk@memsnet.org
> Subject:      RE: [mems-talk] More problems w/ AZ4620.
>
> > I have unsuccessfully attempted to use 4620 recently.  The
> > problem that
> > I have had is a "bubbling" of the resist immediately after exposure.
> > The "bubbles" nucleate in all open areas.  The resist sheds
> > in circular
> > flakes from the open areas - sometimes even before
> > developing.  If there
> > are features surrounded by lots of open area, these features flake off
> > as well.  Has anyone else seen anything like this?
>
> Nitrogen is given off when the resist is exposed.
> Normally it is absorbed in the exposed resist and diffuses away,
> with any left being removed upon developing.
> With thick resists and high exposure powers (mW/cm^2), it can nucleate
> bubbles.
> Try the same dose but with a lower exposure power,
> or do the exposure in pulses to allow time for diffusion.
> Karl Suss had some success with pulsed exposures awhile back.
>
>       --Kirt Williams Agilent Technologies
> _______________________________________________
> mems-talk@memsnet.org mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Addison Engineering
Nano-Master, Inc.
MEMStaff Inc.