Jörn Koblitz
2002-04-05
Dear Peng,

A possible explanation for your observation of increased etch rate with
higher He addition to SF6 etch gas could be, that the He increases the
concentration of free radicals (eigher ionized or non-ionized). Since
SF6 alone doesn't etch anything at all, the etch rate is primarily
controlled by the number (and kind) of reactive species in the process
chamber at a time and the bias voltage at the substrate. The He is
easily ionized and thus can enhance ionization of SF6 itself.

Best regards,

Joern Koblitz

******************************
Joern Koblitz
microFAB Bremen GmbH - the MEMS Wafer Foundry
Universitaetsallee 5
D-28359 Bremen, Germany
Phone: +49 421 24 100 0
Fax: +49 421 24 100 99
eMail: [email protected]
website: www.microfab.de
******************************

-----Original Message-----
From: Peng Yao [mailto:[email protected]]
Posted At: Thursday, March 28, 2002 9:48 PM
Posted To: MEMS-talk
Conversation: [mems-talk] Helium's role in RIE
Subject: [mems-talk] Helium's role in RIE


Hi all,
I am using SF6+He to etch silicon. I thought He will be helpful to get a
smother surface. I fixed all the other parameters like pressure, power,
etching time... and only change the flow rate of SF6 and He. The strange
thing is that the etching speed of SF6:He=10:20 was larger than that of
SF6:He=20:20. (They were etched in same machine and at same day, one
after the other) And also I found that if I fix the gas flow of SF6 and
only change the persentage of He, the etching rate will increase with
increasing the persentage of He. All these seem to indicate that He can
not only cool the photoresist, but also will help the etching. Does
anyone
else has similar experience.
And I am not sure what kind effect of He to side wall, will it make the
process more isotropic or more anisotropic?
Thanks a lot!

Peng Yao
DOEs lab
Electrical Engineering Dept.
Univeristy of delaware
Newark D.E 19716
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
Tanner EDA by Mentor Graphics
University Wafer
Process Variations in Microsystems Manufacturing