Wet etching TiW
2002-04-25
Anke Stock
2002-04-25
___
2002-04-25
Justin Borski
2002-04-25
[email protected]
2002-04-25
Charles Ellis
Wet etching TiW
Justin Borski
2002-04-25
Are you using the usual 10:90 ratio of Ti to Tungsten?  If so, 30% (full
strength) H2O2 by itself should be sufficient to etch the material, unless
it has been exposed to certain other processes which might passivate the
surface.  The etch rate in full strength CMOS grade H2O2 should be about 100
A/min.

Justin C. Borski
MEMS Program Manager
Advanced MicroSensors Inc.


-----Original Message-----
From: Anke Stock [mailto:[email protected]]
Sent: Thursday, April 25, 2002 3:17 AM
To: [email protected]
Subject: [mems-talk] Wet etching TiW


Hello to everybody,
is there someone who has experience in wet etching of TiW? I use a
mixture of HCl and H2O2, but it seems that there are small amounts of
TiW on the wafer after etching. Has someone experiences with parameters
like temperature, time, other mixtures or something else? Many thanks
for your help
Anke
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.
Tanner EDA by Mentor Graphics