A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Plasma etch of BCB
Plasma etch of BCB
2002-04-25
Bill Moffat
Plasma etch of BCB
Bill Moffat
2002-04-25
Lester,
       A number of our customers are using our plasma units for strip and
descum of Polymide and BCB.  A greater number with Polymide so I have numbers
on this process.  Using our microwave down stream unit with 2 KW power for a
single 8 inch wafer with hard baked Polymide approx 8 microns thick the
Polymide is stripped in under 5 minutes.  For descum a lower power and
temperature is used and 500 to 1,000 Angstroms is removed in under 30 seconds.
Various combinations of gas have been used from O2/CF4, O2/SF6 mixtures to gas
mixtures with Nitrogen in.  What sort of plasma system are you using?  Bill
Moffat

-----Original Message-----
From: Lester Lopez [mailto:[email protected]]
Sent: Wednesday, April 24, 2002 12:25 PM
To: [email protected]
Subject: [mems-talk] Plasma etch of BCB


Has anyone attained a controlled plasma
etch of BCB > 1 um per minute using
a CF4/O2 mixture?

If so, what power level and CF4 to O2 ratio
was used?

thanks,

Lester Lopez
University of South Florida
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
The Branford Group
Process Variations in Microsystems Manufacturing
Nano-Master, Inc.