AZ4562 or other thick photoresist
2002-07-02
hzeng
Problems with liftoff(on quartz)
2002-07-03
Balaji Lakshminarayanan
2002-07-03
A.J Pang
2002-07-03
Qingwei Mo
RE: AZ4562 or other thick photoresist
2002-07-05
hzeng
2002-07-08
Anatoli Olkhovets
2002-07-03
Grobe, Dirk
2002-07-08
Danny Hirdes
Problems with liftoff(on quartz)
A.J Pang
2002-07-03
Hi,

It seem that your process does not include the Dehydration bake process before
applying the HMDS.
Also after the the HF dip, I think you should do the DI water dip as well.

Cheers,

AJ


----- Original Message -----
From: "Balaji Lakshminarayanan" 
To: 
Cc: 
Sent: Wednesday, July 03, 2002 1:04 PM
Subject: [mems-talk] Problems with liftoff(on quartz)


> Hi,
>
> I am having problems with developing photoresist on quartz wafer. The
> photoresist is not sticking to the quartz. Has anyone experienced similar
> problems. In particular, with AZ 5214E which i want to use for patterning
> metal using liftoff. The procedure that i followed is
>
> a) 1.50 HF dip for 15sec
> b) spin-on HMDS+AZ5214
> c) soft back @ 90C/60sec
> d) Expose for 8sec
> e) Hard bake for 110C/45sec
> f) Flood expose for 85sec.
>
> I followed the above procedure on glass and it worked well. Any help on the
> same will be appreciated
>
> thanks
>
> bala
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing
Addison Engineering