MEMSnet Home: MEMS-Talk: Si post etch process problems
Si post etch process problems
2003-04-15
Patrick Carlberg
2003-04-17
Kirt & Erika Zipf-Williams
2003-04-16
[email protected]
Si post etch process problems
Kirt & Erika Zipf-Williams
2003-04-17
I've seen the same thing when etching silicon dioxide with a chromium mask.
I think that some of the oxide got sputtered onto the Cr.
The solution was a quick HF dip to remove the oxide before stripping the Cr
mask.

In your case, the solution would be a quick dip in a silicon etchant before
stripping the Cr.
The etchant could be hot KOH or an isotropic silicon etchant.

    --Kirt Williams, Ph.D.        consultant
----- Original Message -----
From: Patrick Carlberg 
To: 
Sent: Tuesday, April 15, 2003 7:27 AM
Subject: [mems-talk] Si post etch process problems


> Dear all
>
> I use RIE with different SF6/O2 ratios to etch Si. I have Cr as an etch
> mask. The problem is that after the etching I cannot remove the Cr etch
> mask. Is there risk for deposition on the Cr-oxide? Can the S molecules
> react somehow? Is there risk for polymerization? Do you have any
> suggestions for solutions?
>
> Sincerely
> Patrick Carlberg
> __________________________________________________
> Patrick Carlberg, Ph.D Student, MSc
> Lund University, Solid State Physics/Nanometer Consortium
> Box 118, SE-221 00 LUND, Sweden
>
> Delivery address: Sölvegatan 14, SE-223 62, LUND, Sweden
> Visiting address: Professorsgatan 1, SE-221 00, LUND, Sweden
>
> Tel:       + 46 46 222 44 95 (office)
> Fax:      + 46 46 222 36 37
> e-mail: [email protected]
> URL: http://www.ftf.lth.se/, http://www.nano.ftf.lth.se
> ___________________________________________________
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
MEMStaff Inc.
Mentor Graphics Corporation
Addison Engineering