MEMSnet Home: MEMS-Talk: electrolessly deposited copper protection
electrolessly deposited copper protection
2004-01-22
Sreelakshmi Yenamandra
2004-01-23
Bill Moffat
2004-01-24
Dipankar Ghosh
2004-01-27
Clements, Jim - Erie
electrolessly deposited copper protection
Dipankar Ghosh
2004-01-24
Hi,
    Could you pls specify the pO2 ( partial pr) that you are using for the Cu
heat treatment.Pls let me know,
           Thanks
                Dipankar
---


---

OFFICE ADDRESS :-

MATERIALS RESEARCH CENTER,
ROOM 322 , RB-1,
1001 CAPABILITY DRIVE,
CENTENNIAL CAMPUS, NCSU,
RALEIGH ,
NC 27695-7919
USA

PH- 919 515 5049
FAX- 919 515 3419








--------- Original Message ---------

DATE: Fri, 23 Jan 2004 09:10:54
From: "Bill Moffat" 
To: "General MEMS discussion" 
Cc:

>Need to know more about your polymer substrate.  A common process used by a
number of my customers is to deposit copper on Polymide then anneal at 300
degrees C and reduce the copper oxide by virtue of the extremely low parts per
billion Oxygen and the temperature.  Polymide will withstand high temperatures.
We have a specialized Polymide bake oven with extremely low Oxygen concentration
that our Silicon wafer customers take up to 450 degrees C.  If your Polymer can
withstand this temperature let me know if you want to test anneal some
structures.  Bill Moffat
>
>-----Original Message-----
>From: Sreelakshmi Yenamandra [mailto:[email protected]]
>Sent: Thursday, January 22, 2004 1:04 PM
>To: [email protected]
>Subject: [mems-talk] electrolessly deposited copper protection
>
>
>Dear All,
>
>I am working on electrolessly deposited copper films on polymer substrates.
After the deposition, I have to protect the copper structures from oxidation. I
know of annealing process but it requires high temperatures which the polymer
substrate might not withstand. Is there any chemical process by which the copper
lines/structures can be protected, without  a change in copper characteristics.
Please suggest.
>
>Sincerely,
>Sreelakshmi Yenamandra
>
>
>
>
>---------------------------------
>Do you Yahoo!?
>Yahoo! SiteBuilder - Free web site building tool. Try it!
>_______________________________________________
>[email protected] mailing list: to unsubscribe or change your list
>options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>Hosted by the MEMS Exchange, providers of MEMS processing services.
>Visit us at http://www.memsnet.org/
>
>_______________________________________________
>[email protected] mailing list: to unsubscribe or change your list
>options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>Hosted by the MEMS Exchange, providers of MEMS processing services.
>Visit us at http://www.memsnet.org/
>



____________________________________________________________
Get advanced SPAM filtering on Webmail or POP Mail ... Get Lycos Mail!
http://login.mail.lycos.com/r/referral?aid=27005


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Nano-Master, Inc.
The Branford Group
Harrick Plasma, Inc.