MEMSnet Home: MEMS-Talk: Help with AZ5214 Info
Help with AZ5214 Info
2004-02-05
Joolien Chee
2004-02-05
Oray Orkun Cellek
Help with AZ5214 Info
Oray Orkun Cellek
2004-02-05
Dear Joolien ,

3 um seems hard ...  I have the following spin-speed vs. thickness data from
Clariant AZ5214E (I hope it is same with AZ5214) data sheet :

2000 rpm 1.98 um
3000 1.62
4000 1.4
5000 1.25
6000 1.14

Best regards,

Oray Orkun Cellek
Research Assistant, Ph. D. Student
Electrical & Electronics Engineering Department
Middle East Technical University
06531 Ankara
Turkey
Tel : +90 312 210 4579
Fax : +90 312 210 1261
e-mail : [email protected]



----- Original Message -----
From: "Joolien Chee" 
To: 
Sent: Thursday, February 05, 2004 6:35 AM
Subject: [mems-talk] Help with AZ5214 Info


> Hi all,
> I am trying to spin AZ 5214 up to 3 microns or more thick. Is there are
> spin-time-thickness plot available for this PR?
> Thanks in advance.
>
> Joolien
>
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
MEMStaff Inc.
Mentor Graphics Corporation
The Branford Group