MEMSnet Home: MEMS-Talk: RIE etching in AlGaAs/GaAs
RIE etching in AlGaAs/GaAs
2004-04-21
Michael Juhl
2004-04-21
Brent Garber (2 parts)
RIE etching in AlGaAs/GaAs
Brent Garber
2004-04-21
Michael,

Nice to get a III-V question now and then.
AlGaAs is a funny material to etch.  If you have any leaks in your chamber
you will grow a dark material believed to be aluminum oxide that stops the
etch.
We have found BCl3 (2 sccm) with Ar (8 sccm) at 20 watts and less than 10
mT
works well for us (we are etching 70% AlGaAs) and is not affected by system
leaks.
AlGaAs less than 15% should etch with Cl2/Ar but roughness is always an
issue with Cl2.

Hope this helps,

Brent

Michael Juhl wrote:

> Hi,
>
>
>
> I need to do a RIE etch in a AlGaAs/GaAs material using Cl2/Ar. I will
> have to etch in depths of about 50nm with etch rates about 30 nm/min.
>
>
>
> If someone has information about recipes that works well with this
> technology please let me know.
>
>
>
> The recipe that I use at the moment is 40 W rf power, 10 mTorr, 3 sccm
> Cl2, 40 sccm Ar. I have problems with surface roughness and unstable
> etching rates.
>
>
>
> Best regards,
>
> Michael Juhl
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
garber.vcf (text/x-vcard, 344 bytes)
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Process Variations in Microsystems Manufacturing
MEMS Technology Review
Mentor Graphics Corporation