Dipankar Ghosh
2004-06-18
Sumant Sood
2004-06-19
Dipankar Ghosh
2004-06-20
MT Klaus Beschorner
Sputtering of Copper
Dipankar Ghosh
2004-06-19
Hi,
        Could you pls let me know what kind of heat treatment you do for Cu.Also
i am using Cu along with Cr as an adhesion layer.Whatever i do Cr always get
oxidized.
     Thanks in advance,
            Dipankar Ghosh


---

OFFICE ADDRESS :-

MATERIALS RESEARCH CENTER,
ROOM 322 , RB-1,
1001 CAPABILITY DRIVE,
CENTENNIAL CAMPUS, NCSU,
RALEIGH ,
NC 27695-7919
USA

PH- 919 515 5049
FAX- 919 515 3419








--------- Original Message ---------

DATE: Fri, 18 Jun 2004 18:18:47
From: MT Klaus Beschorner 
To: [email protected]
Cc:

> >I am trying to sputter thick Cu ( 1 um) in a DC sputtering system.my
> >sputtering conditions are as follows :-
> >base pr- 10 exp(-6) torr
> >chamber pr -10 m torr
> >Ar gas flow - 10 sccm.
> >power - 250 W
> >Target to substrate distance - 5 cm.
> >
> >my problem is that the resistivity of my deposited Cu is very high (24
> >micro ohm cm) which is about 15 times the bulk resistivity of Cu( 1.6
> >micro ohm cm).
>
>With your base pressure level and low power, dep. time is very long
>and a lot of contaminants get incorporated in the film. Leading edge
>CMOS fabs use b.p. <1E-8 torr, 5-10kW power. Even then, as-deposited
>Cu resistance is higher than bulk (~2.5µOhmcm), subsequent anneal will
>reduce it to <2µOhmcm.
>
>best regards,
>klaus
>
>--
>Klaus Beschorner
>Metron Technology Europe, PVD (Eclipse) Process Manager
>Drosselweg 6,71120 Grafenau,Germany. Tel +49-7033-45683
>
>
>_______________________________________________
>[email protected] mailing list: to unsubscribe or change your list
>options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>Hosted by the MEMS Exchange, providers of MEMS processing services.
>Visit us at http://www.memsnet.org/
>



____________________________________________________________
Find what you are looking for with the Lycos Yellow Pages
http://r.lycos.com/r/yp_emailfooter/http://yellowpages.lycos.com/default.asp?SRC
=lycos10

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
Nano-Master, Inc.
The Branford Group
Process Variations in Microsystems Manufacturing