MEMSnet Home: MEMS-Talk: removing AZ5214
removing AZ5214
2004-07-25
William Lanford-Crick
2004-07-26
Paolo Tassini
removing AZ5214
Paolo Tassini
2004-07-26
Hi!
In our process, we use postbake at 115°C for 90seconds
and flood exposure at 17mW/cm2 for 10seconds.
For removing your resist you can also use oxygen plasma,
if your devices can withstand it.

Ing. Paolo Tassini
Sezione MAT-NANO
Centro Ricerche ENEA Portici



> Hi Group,
> I know it sounds like a trivial question, but I am recently
> having great difficulty in removing AZ5214 photoresist that
> has undergone image reversal.  Even after no further
> processing beyond PR developing, I cannot easily strip the
> resist in Acetone.  Boiling acetone seems to have little
> effect on the resist. This is a standard procedure which I
> have not until recently had any problems with.
>
> See process below.  There is not prblem when I do the
> positive-image process.  Should I try lower postbake temp or
> lower flood exposure?  Why do you think I cannot remove the
> resist in acetone??  Thanks!
>
> Process is as follows:
> Spin AZ5214E PR at 5000 RPM / 30 sec.
> prebake at 110deg. C / 30 sec.
> expose 8 sec. in KS - MJB-3 (I don't know the intensity
> offhand)
> Postbake at 125deg. C / 60 sec.
> Flood expose 330 mJ/cm^2
> Develop 45 - 50 sec. in AZ327 MIF.
>



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
Mentor Graphics Corporation
Process Variations in Microsystems Manufacturing
MEMS Technology Review